Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.
This is the free Material Data Center Datasheet of Makrolon® 2405 RE - PC - Covestro Deutschland AG
Material Data Center offers the following functions for Makrolon® 2405 RE:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces
Check here, which other Makrolon datasheets, application examples or technical articles are available in Material Data Center
Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our
disclaimer.
Informação do produto
- MVR (300 °C/1.2 kg) 19 cm³/10 min
- general purpose
- low viscosity
- easy release
Características de processamento/físicas | Valor | Unidade | Método de ensaio |
ISO Dados |
Índice de fluidez volumétrico, MVR |
19 |
cm³/10min |
ISO 1133 |
Temperatura |
300 |
°C |
- |
Carga |
1.2 |
kg |
- |
Índice de fluidez, MFI |
20 |
g/10min |
ISO 1133 |
Temperatura |
300 |
°C |
- |
Carga |
1.2 |
kg |
- |
Contração após a moldagem, paralelo |
0.7 |
% |
ISO 294-4, 2577 |
Contração após a moldagem, perpendicular |
0.7 |
% |
ISO 294-4, 2577 |
Propriedades mecânicas | Valor | Unidade | Método de ensaio |
ISO Dados |
Módulo de tração |
2400 |
MPa |
ISO 527 |
Tensão no escoamento |
65 |
MPa |
ISO 527 |
Deformação no escoamento |
6 |
% |
ISO 527 |
Deformação nominal na ruptura |
>50 |
% |
ISO 527 |
Módulo de flexão, 23°C |
2350 |
MPa |
ISO 178 |
Resistência à flexão |
97 |
MPa |
ISO 178 |
Módulo de tensão de fluência, 1h |
2200 |
MPa |
ISO 899-1 |
Módulo de tensão de fluência, 1000h |
1900 |
MPa |
ISO 899-1 |
Resistência ao impacto Charpy , +23°C |
N |
kJ/m² |
ISO 179/1eU |
Res. impacto Charpy c/entalhe, +23°C, 3mm |
65 |
kJ/m² |
ISO 179/1eA |
Type of failure |
P |
- |
- |
Res. impacto Charpy c/entalhe, -30°C, 3mm |
14 |
kJ/m² |
ISO 179/1eA |
Type of failure |
C |
- |
- |
Impacto Izod com entalhe, +23°C |
65 |
kJ/m² |
ISO 180/1A |
Impacto Izod com entalhe |
15 |
kJ/m² |
ISO 180/1A |
Temperatura |
-30 |
°C |
- |
Perfuração - força máxima, +23°C |
5100 |
N |
ISO 6603-2 |
Perfuração - força máxima, -30°C |
6000 |
N |
ISO 6603-2 |
Energia de perfuração, +23°C |
55 |
J |
ISO 6603-2 |
Energia de perfuração, -30°C |
65 |
J |
ISO 6603-2 |
Ball indentation hardness |
115 |
MPa |
ISO 2039-1 |
Propriedades térmicas | Valor | Unidade | Método de ensaio |
ISO Dados |
Temp. de transição vítrea, 10°C/min |
144 |
°C |
ISO 11357-1/-2 |
Temperatura de deflexão térmica, 1.80 MPa |
124 |
°C |
ISO 75-1/-2 |
Temperatura de deflexão térmica, 0.45 MPa |
137 |
°C |
ISO 75-1/-2 |
Temperatura de amolecimento Vicat, B |
145 |
°C |
ISO 306 |
Coef. de expansão térmica linear, paralelo |
65 |
E-6/K |
ISO 11359-1/-2 |
Coef. de expansão térmica linear, perpend. |
65 |
E-6/K |
ISO 11359-1/-2 |
Flamabilidade a espessura h |
V-2 |
class |
IEC 60695-11-10 |
Espessuras do tubo de teste |
0.8 |
mm |
- |
Flamabilidade conforme índice de oxigênio |
27 |
% |
ISO 4589-1/-2 |
Glow Wire Flammability Index (GWFI) |
850 |
°C |
IEC 60695-2-12 |
GWFI - thickness tested (1) |
0.75 |
mm |
- |
Glow Wire Flammability Index (GWFI) |
875 |
°C |
IEC 60695-2-12 |
GWFI - thickness tested (2) |
1.5 |
mm |
- |
Glow Wire Flammability Index (GWFI) |
930 |
°C |
IEC 60695-2-12 |
GWFI - thickness tested (3) |
3 |
mm |
- |
Glow Wire Ignition Temperature (GWIT) |
875 |
°C |
IEC 60695-2-13 |
GWIT - thickness tested (1) |
0.75 |
mm |
- |
Glow Wire Ignition Temperature (GWIT) |
875 |
°C |
IEC 60695-2-13 |
GWIT - thickness tested (2) |
1 |
mm |
- |
Glow Wire Ignition Temperature (GWIT) |
875 |
°C |
IEC 60695-2-13 |
GWIT - thickness tested (3) |
1.5 |
mm |
- |
Propriedades elétricas | Valor | Unidade | Método de ensaio |
ISO Dados |
Constante dielétrica, 100Hz |
3.1 |
- |
IEC 62631-2-1 |
Constante dielétrica, 1MHz |
3 |
- |
IEC 62631-2-1 |
Fator de dissipação dielétrica, 100Hz |
5 |
E-4 |
IEC 62631-2-1 |
Fator de dissipação dielétrica, 1MHz |
90 |
E-4 |
IEC 62631-2-1 |
Resistividade volumétrica específica |
>1E13 |
Ohm*m |
IEC 62631-3-1 |
Resistividade superficial específica |
>1E15 |
Ohm |
IEC 62631-3-2 |
Resistência elétrica |
34 |
kV/mm |
IEC 60243-1 |
Índice comparativo de linha de fuga |
250 |
- |
IEC 60112 |
Propriedades ópticas | Valor | Unidade | Método de ensaio |
ISO Data |
Haze |
80 |
- |
ISO 14782 |
Transmitância luminosa |
89 |
% |
ISO 13468-1, -2 |
Outras propriedades | Valor | Unidade | Método de ensaio |
Absorção de água |
0.3 |
% |
Sim. to ISO 62 |
Absorção de umidade |
0.12 |
% |
Sim. to ISO 62 |
Densidade |
1200 |
kg/m³ |
ISO 1183 |
Bulk density |
660 |
kg/m³ |
- |
Propriedades do filme | Valor | Unidade | Método de ensaio |
ISO Dados |
WVTR, 23°C/85%r.h. |
15 |
g/(m²*d) |
ISO 15106-1/-2 |
Espessura de corpo de prova |
0.1 |
mm |
- |
Produção de amostra para teste | Valor | Unidade | Método de ensaio |
ISO Dados |
Moldagem por injeção, temperatura da massa |
280 |
°C |
ISO 294 |
Moldagem por injeção, temperatura do molde |
80 |
°C |
ISO 294 |
Moldagem por injeção, velocidade de injeção |
200 |
mm/s |
ISO 294 |
Recomendação de processamento Moldagem por injeção | Valor | Unidade | Método de ensaio |
Pré-secagem - temperatura |
120 |
°C |
- |
Pré-secagem - tempo |
2 - 3 |
h |
- |
Umidade do processamento |
≤0.02 |
% |
- |
Temperatura da massa |
280 - 320 |
°C |
- |
Temperatura do molde |
80 - 120 |
°C |
- |
Zona 1 |
250 - 260 |
°C |
- |
Zona 2 |
270 - 280 |
°C |
- |
Zona 3 |
280 - 290 |
°C |
- |
Temperatura do bico |
290 - 300 |
°C |
- |
Contrapressão |
5 - 15 |
MPa |
- |
Características
Processamento
Moldagem por injeção
Forma de entrega
Granulos
Aditivos
Desmoldante
Características especiais
Transparente, Opaque, Translucent
Certifications
ISCC Plus
Aplicaciones
Polivalente
Disponibilidade regional
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com
Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.
Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.