Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.
This is the free Material Data Center Datasheet of Makrolon® 2405 RE - PC - Covestro Deutschland AG
Material Data Center offers the following functions for Makrolon® 2405 RE:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces
Check here, which other Makrolon datasheets, application examples or technical articles are available in Material Data Center
Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our
disclaimer.
Testo del prodotto
- MVR (300 °C/1.2 kg) 19 cm³/10 min
- general purpose
- low viscosity
- easy release
Caratteristiche Fisiche | Valore | Unitá | Norma del test |
ISO Data |
Indice di fusione di volume, MVR |
19 |
cm³/10min |
ISO 1133 |
Temperatura |
300 |
°C |
- |
Carico |
1.2 |
kg |
- |
Indice di Fluiditá, MFI |
20 |
g/10min |
ISO 1133 |
Temperatura |
300 |
°C |
- |
Carico |
1.2 |
kg |
- |
Ritiro di stampaggio, parallelo |
0.7 |
% |
ISO 294-4, 2577 |
Ritiro di stampaggio, perpendicolare |
0.7 |
% |
ISO 294-4, 2577 |
Proprietà Meccaniche | Valore | Unitá | Norma del test |
ISO Data |
Modulo a trazione |
2400 |
MPa |
ISO 527 |
Carico unitario a trazione |
65 |
MPa |
ISO 527 |
Deformazione a snervamento |
6 |
% |
ISO 527 |
Deformazione nominale a rottura |
>50 |
% |
ISO 527 |
Modulo a flessione, 23°C |
2350 |
MPa |
ISO 178 |
Resistenza alla flessione |
97 |
MPa |
ISO 178 |
Modulo di scorrimento a trazione, 1h |
2200 |
MPa |
ISO 899-1 |
Modulo di scorrimento a trazione, 1000h |
1900 |
MPa |
ISO 899-1 |
Resistenza all'urto Charpy, +23°C |
N |
kJ/m² |
ISO 179/1eU |
Resist. urto Charpy con intaglio, +23°C, 3mm |
65 |
kJ/m² |
ISO 179/1eA |
Type of failure |
P |
- |
- |
Resist. urto Charpy con intaglio, -30°C, 3mm |
14 |
kJ/m² |
ISO 179/1eA |
Type of failure |
C |
- |
- |
Resistenza all'urto Izod con intaglio, +23°C |
65 |
kJ/m² |
ISO 180/1A |
Resistenza all'urto Izod con intaglio |
15 |
kJ/m² |
ISO 180/1A |
Temperatura |
-30 |
°C |
- |
Perforazione-forza massima, +23°C |
5100 |
N |
ISO 6603-2 |
Perforazione-forza massima, -30°C |
6000 |
N |
ISO 6603-2 |
Energia di perforazione, +23°C |
55 |
J |
ISO 6603-2 |
Energia di perforazione, -30°C |
65 |
J |
ISO 6603-2 |
Ball indentation hardness |
115 |
MPa |
ISO 2039-1 |
Proprietà Termiche | Valore | Unitá | Norma del test |
ISO Data |
Temperatura di transizione vetrosa, 10°C/min |
144 |
°C |
ISO 11357-1/-2 |
Temp.di inflessione sotto carico, 1.80 MPa |
124 |
°C |
ISO 75-1/-2 |
Temp.di inflessione sotto carico, 0.45 MPa |
137 |
°C |
ISO 75-1/-2 |
Temp.di rammollimento Vicat, B |
145 |
°C |
ISO 306 |
Coeff.di dilatazione termica lin., parallelo |
65 |
E-6/K |
ISO 11359-1/-2 |
Coeff.di dilatazione termica lin., perpend. |
65 |
E-6/K |
ISO 11359-1/-2 |
Reazione al fuoco a spessore h |
V-2 |
class |
IEC 60695-11-10 |
Spessore provato |
0.8 |
mm |
- |
Indice di ossigeno |
27 |
% |
ISO 4589-1/-2 |
Glow Wire Flammability Index (GWFI) |
850 |
°C |
IEC 60695-2-12 |
GWFI - thickness tested (1) |
0.75 |
mm |
- |
Glow Wire Flammability Index (GWFI) |
875 |
°C |
IEC 60695-2-12 |
GWFI - thickness tested (2) |
1.5 |
mm |
- |
Glow Wire Flammability Index (GWFI) |
930 |
°C |
IEC 60695-2-12 |
GWFI - thickness tested (3) |
3 |
mm |
- |
Glow Wire Ignition Temperature (GWIT) |
875 |
°C |
IEC 60695-2-13 |
GWIT - thickness tested (1) |
0.75 |
mm |
- |
Glow Wire Ignition Temperature (GWIT) |
875 |
°C |
IEC 60695-2-13 |
GWIT - thickness tested (2) |
1 |
mm |
- |
Glow Wire Ignition Temperature (GWIT) |
875 |
°C |
IEC 60695-2-13 |
GWIT - thickness tested (3) |
1.5 |
mm |
- |
Proprietà Elettriche | Valore | Unitá | Norma del test |
ISO Data |
Costante dielettrica relativa, 100Hz |
3.1 |
- |
IEC 62631-2-1 |
Costante dielettrica relativa, 1MHz |
3 |
- |
IEC 62631-2-1 |
Fattore di dissipazione, 100Hz |
5 |
E-4 |
IEC 62631-2-1 |
Fattore di dissipazione, 1MHz |
90 |
E-4 |
IEC 62631-2-1 |
Resistività volumica |
>1E13 |
Ohm*m |
IEC 62631-3-1 |
Resistività superficiale |
>1E15 |
Ohm |
IEC 62631-3-2 |
Rigidità dielettrica |
34 |
kV/mm |
IEC 60243-1 |
Res. Alle correnti striscianti superficiali |
250 |
- |
IEC 60112 |
Proprietà Ottiche | Valore | Unitá | Norma del test |
ISO Data |
Opacità |
80 |
- |
ISO 14782 |
Trasmittanza luminosa |
89 |
% |
ISO 13468-1, -2 |
Altre Proprietà | Valore | Unitá | Norma del test |
Assorbimento d'acqua |
0.3 |
% |
Sim. alla ISO 62 |
Assorbimento d'umidità |
0.12 |
% |
Sim. alla ISO 62 |
Massa volumica |
1200 |
kg/m³ |
ISO 1183 |
Bulk density |
660 |
kg/m³ |
- |
Proprietà Meccaniche (Film) | Valore | Unitá | Norma del test |
ISO Data |
WVTR, 23°C/85%r.h. |
15 |
g/(m²*d) |
ISO 15106-1/-2 |
Spessore del provino |
0.1 |
mm |
- |
Preparazione Provette | Valore | Unitá | Norma del test |
ISO Data |
Stamp. ad Iniezione, temp. di fusione |
280 |
°C |
ISO 294 |
Stamp. ad Iniezione, temperatura dello stampo |
80 |
°C |
ISO 294 |
Stamp. ad Iniezione, velocità media d'iniezione |
200 |
mm/s |
ISO 294 |
Raccomandazione de Processabilità Stampaggio ad Iniezione | Valore | Unitá | Norma del test |
Pre-essiccamento - Temperatura |
120 |
°C |
- |
Pre-essiccamento - Tempo |
2 - 3 |
h |
- |
Umidità del Processo |
≤0.02 |
% |
- |
Temperatura di fusione |
280 - 320 |
°C |
- |
Temperatura dello stampo |
80 - 120 |
°C |
- |
Zona 1 |
250 - 260 |
°C |
- |
Zona 2 |
270 - 280 |
°C |
- |
Zona 3 |
280 - 290 |
°C |
- |
Temperatura dell ugello |
290 - 300 |
°C |
- |
Contropressione |
5 - 15 |
MPa |
- |
Caratteristiche
Processabilità e Forma di Forni
Stampaggio ad Iniezione
Forma fisica disponibile
Pellet
Additivi
Agente di distacco
Caratteristiche speciali
Trasparente, Opaque, Translucent
Certifications
ISCC Plus
Applicazioni
Polivalente
Disponibilità geografica
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com