Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of PLEXIGLAS® Resist zk50 - PMMA-I - Röhm GmbH

Material Data Center offers the following functions for PLEXIGLAS® Resist zk50:
unit conversion, PDF datasheet print, comparison with other plastics, flow length calculation, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Plexiglas datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informations produit

Productprofil:

PLEXIGLAS® Resist zk50 is an amorphous, impact-modified thermoplastic molding compound (PMMA-I).

 

Typical properties of impact-modified PLEXIGLAS® molding compounds are

 

  • excellent transmission and clarity
  • brilliant appearance
  • the pleasant feel and sound of the moldings.

 

PLEXIGLAS® Resist zk50 is characterized by the following special properties:

 

  • maximum break resistance and impact strength
  • improved resistance to stress cracking
  • certified dishwasher resistance

Application:

Used for injection molding. Profile extrusion or coextrusion are also possible

Example:

lighting fixtures, writing and drawing utensils, domestic appliances and sanitaryware

Processing:

PLEXIGLAS® Resist zk molding compounds can be processed on machines with 3-zone general purpose screws for engineering thermoplastics.

Physical Form / Packaging:

PLEXIGLAS® Resist zk molding compounds are supplied as pellets of uniform size, packaged in 25kg polyethylene bags or 500kg boxes with PE lining; other packaging on request.

Caractéristiques des transformations/physiquesValeurUnitéNorme du test
ISO Data
Indice de fluidité à chaud en volume, MVR 0.1 cm³/10min ISO 1133
Température 230 °C -
Charge 3.8 kg -
Densité du fondu 1040 kg/m³ -
Conductivité thermique du fondu 0.19 W/(m K) -
Chaleur spécifique du fondu 2440 J/(kg K) -
Diffusivité thermique 7.49E-8 m²/s -
Température d'éjection 55 °C -
Propriétés mécaniquesValeurUnitéNorme du test
ISO Data
Module en traction 950 MPa ISO 527
Contrainte d'écoulement 25 MPa ISO 527
Déformation au seuil d'écoulement 5 % ISO 527
Déformation nominale à la rupture >50 % ISO 527
Module de fluage en traction, 1h 900 MPa ISO 899-1
Module de fluage en traction, 1000h 600 MPa ISO 899-1
Résistance au choc Charpy, +23°C N kJ/m² ISO 179/1eU
Résistance au choc Charpy (entaillé), +23°C 13 kJ/m² ISO 179/1eA
Propriétés thermiquesValeurUnitéNorme du test
ISO Data
Température de transition vitreuse, 10°C/min 115 °C ISO 11357-1/-2
Température de fléchissement s/chrg, 1.80 MPa 70 °C ISO 75-1/-2
Température de fléchissement s/chrg, 0.45 MPa 73 °C ISO 75-1/-2
Température de ramolliss. Vicat, B 75 °C ISO 306
Coeffic. de dilatation therm. linéique, parallèle 150 E-6/K ISO 11359-1/-2
Inflammabilité ep. nom. 1.5 mm HB class IEC 60695-11-10
Epaisseur de l'éprouvette 1.6 mm -
Yellow Card disponible oui - -
Aptitude à l'allumage 17.5 % ISO 4589-1/-2
Propriétés électriquesValeurUnitéNorme du test
ISO Data
Permittivité relative, 100Hz 4 - IEC 62631-2-1
Permittivité relative, 1MHz 2.9 - IEC 62631-2-1
Facteur de pertes, 100Hz 400 E-4 IEC 62631-2-1
Facteur de pertes, 1MHz 400 E-4 IEC 62631-2-1
Résistivité transversale >1E13 Ohm*m IEC 62631-3-1
Résistivité superficielle 1E13 Ohm IEC 62631-3-2
Indice de résistance au cheminement 600 - IEC 60112
Propriétés optiquesValeurUnitéNorme du test
ISO Data
Transmittance 89 % ISO 13468-1, -2
Propriétés diversesValeurUnitéNorme du test
Absorption d'eau 1.2 % Sim. to ISO 62
Absorption d'humidité 0.4 % Sim. to ISO 62
Masse volumique 1120 kg/m³ ISO 1183
Préparation et conditionnement des éprouvettesValeurUnitéNorme du test
ISO Data
Injection, température de la matière fondue 265 °C ISO 294
Injection, température du moule 40 °C ISO 294
Injection, vitesse d'injection 195 mm/s ISO 294
Fonctions
Viscosité / Vitesse de cisaillement , PLEXIGLAS® Resist zk50, PMMA-I, Röhm
Contrainte de cisaillement / Vit. de cisaillement , PLEXIGLAS® Resist zk50, PMMA-I, Röhm
Module de cisaillement dynamique / Température , PLEXIGLAS® Resist zk50, PMMA-I, Röhm
Contrainte / Déformation , PLEXIGLAS® Resist zk50, PMMA-I, Röhm
Module sécant / Déformation , PLEXIGLAS® Resist zk50, PMMA-I, Röhm
Contrainte / Déformation (isochrone) 23°C, PLEXIGLAS® Resist zk50, PMMA-I, Röhm
Module de fluage / Temps 23°C, PLEXIGLAS® Resist zk50, PMMA-I, Röhm
Courbe de fluage 23°C, PLEXIGLAS® Resist zk50, PMMA-I, Röhm
Module de traction / Température , PLEXIGLAS® Resist zk50, PMMA-I, Röhm
Caractéristiques
Transformation
Moulage par injection, Extrusion de films, Extrusion de profilés, Extrusion de plaques, Extrusion (autres)
Conditionnement
Granulés
Additifs
Agent de démoulage
Propriétés spéciales
Modifié choc, Stabilisé à la lumière, Stabilisé aux intempéries, Transparent
Caractéristiques
Amorphe
Résistance Chimique
Fissuration à l’environnement
Disponibilité régionale
Amérique du nord, Europe, Asia Pacific, South and Central America, Proche-Orient/Afrique
Autres informations
Moulages par injection
PREPROCESSING
Predrying temperature: max. 70 °C
Predrying time in a desiccant-type drier: 2 - 3 h
PROCESSING
Melt temperature: 230 - 240°C
Mold temperature:50 - 70°C
Extrusion de profilés
PREPROCESSING
Predrying temperature: max. 70 °C
Predrying time in a desiccant-type drier: 2 - 3 h
PROCESSING
Melt temperature: 230 - 240 °C
Die temperature: 230 - 240 °C
Extrusion de feuilles
PREPROCESSING
Predrying temperature: max. 70 °C
Predrying time in a desiccant-type drier: 2 - 3 h
PROCESSING
Melt temperature: 230 - 240 °C
Die temperature: 230 - 240 °C
Conditions générales
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.