Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of NORYL™ Resin 7310 - Asia - (PPE+PS) - Saudi Basic Industries Corporation (SABIC)

Material Data Center offers the following functions for NORYL™ Resin 7310 - Asia:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Noryl datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
NORYL™ 7310 resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This injection moldable grade exhibits good surface appearance, high ductility, and good impact resistance along with low moisture absorption, creep resistance, dimensional stability, and hydrolytic stability. NORYL 7310 resin is an excellent candidate for a variety of applications.

UL Yellow Card Link E45587-237006
Caracteristicas de procesamiento y fisicasValorUnidadesMétodo de ensayo
ISO Data
Indice de fluidez volumétrico, MVR 12 cm³/10min ISO 1133
Temperatura 280 °C -
Carga 5 kg -
ASTM Data
Índice de fluidez, MFI 11 g/10min ASTM D 1238
Temperatura 280 °C -
Carga 5 kg -
Propiedades mecánicasValorUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 2100 MPa ISO 527
Esfuerzo de fluencia 40 MPa ISO 527
Alarg. en límite elástico 70 % ISO 527
Resistencia a la tracción 40 MPa ISO 527
Alargamiento a rotura 50 % ISO 527
Modulo de Flexión 2300 MPa ISO 178
Resistencia al impacto Charpy c/entalla, +23°C 13 kJ/m² ISO 179/1eA
Izod impact strength, +23°C, 4mm 60 kJ/m² ISO 180/1U
Izod impact strength, -30°C, 4mm 55 kJ/m² ISO 180/1U
Res. impacto Izod c/entalla, +23°C, 4mm 16 kJ/m² ISO 180/1A
Res. impacto Izod c/entalla, -30°C, 4mm 11 kJ/m² ISO 180/1A
ASTM Data
Módulo de tracción 2400 MPa ASTM D 638
Esfuerzo de fluencia a tracción 54 MPa ASTM D 638
Esfuerzo de fractura a tracción 45 MPa ASTM D 638
Alargamiento a la fluencia 4 % ASTM D 638
Alargamiento a la rotura 30 % ASTM D 638
Módulo de flexión 2100 MPa ASTM D 790
Resistencia al impacto Izod con entalla, 1/8 in 150 J/m ASTM D 256
Resistencia al impacto Izod con entalla, baja temperatura 120 J/m ASTM D 256
Temperatura -30 °C -
Resistencia al impacto Izod, 1/8 in 800 J/m ASTM D 256
Propiedades térmicasValorUnidadesMétodo de ensayo
ISO Data
Estabilidad al calor, 1.80 MPa 112 °C ISO 75-1/-2
Temp. reblandecimiento Vicat, B 133 °C ISO 306
Temp. reblandecimiento Vicat, 120°C/h 50N 135 °C ISO 306
Combustibilidad a 1.5mm esp. nom. HB class IEC 60695-11-10
Espesores de probeta 1.5 mm -
ASTM Data
Estabilidad al calor @ 264 psi 110 °C ASTM D 648
Temperatura Vicat 133 °C ASTM D 1525
Otras propiedadesValorUnidadesMétodo de ensayo
Densidad 1080 kg/m³ ASTM D 792
Recomendación para procesamiento Moldeo por inyecciónValorUnidadesMétodo de ensayo
Temperatura de pre-secado 105 - 110 °C -
Tiempo de pre-secado 3 - 4 h -
Humedad de procesamiento ≤0.02 % -
Temperatura de la masa 280 - 310 °C -
Temperatura del molde 75 - 105 °C -
Zona 1 250 - 300 °C -
Zona 2 260 - 305 °C -
Zona 3 270 - 310 °C -
Velocidad de giro de husillo 20 - 100 rpm -
Contrapresión 0.3 - 0.7 MPa -
Características
Procesamiento y forma de entrega
Moldeo por inyección
Resistencia quimica
Estabilidad hidrolitica
Applicaciones
Automotriz
Disponibilidad regional
Asia Pacifico
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.