Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Grilamid TR 90 UV LS natural - PAMACM12 - EMS-GRIVORY | a unit of EMS-CHEMIE AG

Material Data Center offers the following functions for Grilamid TR 90 UV LS natural:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Grilamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Texto del producto
Product-nomenclature: ISO 16396-PAMACM12,,GTL1,C14-020

 

Product Attributes

  Highly transparent, Improved UV resistance (outdoor use)

Markets

  Automotive
  Automotive electr. and electronics, lighting, Cooling and climate control, Fuel systems,
Powertrain and Chassis, Interior, Exterior
  Electricals & Electronics
  Electrical equipment, Lighting
  Industry & Consumer goods
  Hydraulics & Pneumatics, Mechanical Engineering, Sports & Leisure, Tools & Accessories

Approvals

  Food Contact
  EU Requirements, FDA
Caracteristicas de procesamiento y fisicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Contracción posterior al moldeo, paralelo 0.7 / * % ISO 294-4, 2577
Contracción posterior al moldeo, normal 0.8 / * % ISO 294-4, 2577
Propiedades mecánicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Módulo de tracción 1600 / 1600 MPa ISO 527
Esfuerzo de fluencia 60 / 60 MPa ISO 527
Alarg. en límite elástico 8 / 6 % ISO 527
Alarg. nominal a rotura >50 / >50 % ISO 527
Resistencia al impacto Charpy, +23°C N / N kJ/m² ISO 179/1eU
Resistencia al impacto Charpy, -30°C N / N kJ/m² ISO 179/1eU
Resistencia al impacto Charpy c/entalla, +23°C 13 / 13 kJ/m² ISO 179/1eA
Resistencia al impacto Charpy c/entalla, -30°C 12 / 12 kJ/m² ISO 179/1eA
Dureza Shore D 81 / * - ISO 7619-1
Propiedades térmicasSeco / CondUnidadesMétodo de ensayo
ISO Data
Temp. de transición vítrea, 10°C/min 155 / * °C ISO 11357-1/-2
Estabilidad al calor, 1.80 MPa 115 / * °C ISO 75-1/-2
Estabilidad al calor, 0.45 MPa 135 / * °C ISO 75-1/-2
Coef.de expansión térmica lineal, paralelo 90 / * E-6/K ISO 11359-1/-2
Coef.de expansión térmica lineal, normal 90 / * E-6/K ISO 11359-1/-2
Combustibilidad a espesor h HB / * class IEC 60695-11-10
Espesores de probeta 0.8 / * mm -
Propiedades eléctricasSeco / CondUnidadesMétodo de ensayo
ISO Data
Resistividad volumétrica específica 1E11 / 1E11 Ohm*m IEC 62631-3-1
Resistividad superficial específica * / 1E12 Ohm IEC 62631-3-2
Resistencia dieléctrica 34 / 34 kV/mm IEC 60243-1
Indice comparativo de linea de fuga - / 600 - IEC 60112
Otras propiedadesSeco / CondUnidadesMétodo de ensayo
Absorción de agua 3 / * % Sim. to ISO 62
Absorción de humedad 1.5 / * % Sim. to ISO 62
Densidad 1000 / - kg/m³ ISO 1183
Funciones
Viscosidad-velocidad de cizallamiento , Grilamid TR 90 UV LS natural, PAMACM12, EMS-GRIVORY
Tensión de cizalla-velocidad de cizalla , Grilamid TR 90 UV LS natural, PAMACM12, EMS-GRIVORY
Módulo de cizallamiento dinámico-temperatura , Grilamid TR 90 UV LS natural (Cond), PAMACM12, EMS-GRIVORY
Esfuerzo-alargamiento , Grilamid TR 90 UV LS natural (Cond), PAMACM12, EMS-GRIVORY
Módulo secante-alargamiento , Grilamid TR 90 UV LS natural (Cond), PAMACM12, EMS-GRIVORY
Volumen especifico-temperatura (pvT) , Grilamid TR 90 UV LS natural, PAMACM12, EMS-GRIVORY
Características
Procesamiento y forma de entrega
Moldeo por inyección, Otros tipos de extrusión
Forma de suministro
Granulado, Color natural
Aditivos
Desmoldeante
Características especiales
Estable a la luz, Estable contra rayos U.V./interperie, Transparente
Certifications
Contacto con alimentos, Aprobado por el FDA 21 CFR
Applicaciones
Automotriz, Electrica, Equipos deportivos
Disponibilidad regional
Demás información
Moldeo por inyección
PREPROCESSING
Max. water content : <= 0.08 %
PROCESSING
Melt temperature : 270 °C
Mould wall temperature : 60-80 °C
Holding pressure : 300-600 bar
Screw : 50-100 rpm
Back pressure : 1-15 bar
Injection speed : 3
(1=slow, 3=medium, 5=fast)

Please consider the information about the application of the materials.
Otros tipos de extrusión
-- PIPE EXTRUSION --
-- SHEATING --
PROCESSING
Melt temperature : 250-270 °C
Feeding bush : 60-90
Barrel temp. profile : 240-250 °C
Head temp. : 250-240 °C

Please consider the information about the application of the materials.
Resistencia a medios químicos
Acidos
Ácido acético (5% por masa) (23°C)
Solución ácido cítrico (10% por masa) (23°C)
Ácido láctico (10% por masa) (23°C)
Ácido clorhídrico (36% por masa) (23°C)
Ácido nítrico (40% por masa) (23°C)
Ácido sulfúrico (38% por masa) (23°C)
Ácido sulfúrico (5% por masa) (23°C)
Solución ácido crómico (40% por masa) (23°C)
Bases
Solución de hidróxido de sodio (35% por masa) (23°C)
Solución de hidróxido de sodio (1% por masa) (23°C)
Solución de hidróxido de amónio (10% por masa) (23°C)
Alcoholes
Alcohol isopropílico (23°C)
Metanol (23°C)
Etanol (23°C)
Hidrocarburos
N-hexano (23°C)
Tolueno (23°C)
Iso-octano (23°C)
Cetonas
Acetona (23°C)
Éteres
Dietil éter (23°C)
Aceites minerales
SAE 10w40 aceite motor multigrado (23°C)
SAE 10w40 aceite motor multigrado (130°C)
SAE 80/90 aceite para engranajes hipocíclicos (130°C)
Aceite aislante (23°C)
Combustibles normales
ISO 1817 líquido 1 (60°C)
ISO 1817 líquido 2 (60°C)
ISO 1817 líquido 3 (60°C)
ISO 1817 líquido 4 (60°C)
Combustible normal sin alcohol (pref. ISO 1817 líquido C) (23°C)
Combustible normal con alcohol (pref. ISO 1817 líquido 4) (23°C)
Combustible diesel (pref. ISO 1817 líquido F) (23°C)
Combustible diesel (pref. ISO 1817 líquido F) (90°C)
Combustible diesel (pref. ISO 1817 líquido F) (>90°C)
Soluciones de sal
Solución de cloruro de sodio (10% por masa) (23°C)
Solución de hipoclorito de sodio (10% por masa) (23°C)
Solución de carbonato sódico (20% por masa) (23°C)
Solución de carbonato sódico (2% por masa) (23°C)
Solución de cloruro de cinc (50% por masa) (23°C)
Otros
Acetato etílico (23°C)
Agua oxigenada (23°C)
Fluido de freno DOT no. 4 (130°C)
Glicol etilénico (50% por masa) en agua (108°C)
1% etanol dnonylphenoxy-polyethyleneoxy en agua (23°C)
50% ácido oleico + 50% aceite de oliva (23°C)
Agua (23°C)
Agua desionizada (90°C)
Solución de fenol (5% por masa) (23°C)
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com