Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Xyron™ 540V - (PPE+PS) - Asahi Kasei

Material Data Center offers the following functions for Xyron™ 540V:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Xyron datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Strength 60 MPa ISO 527-1/-2
Charpy notched impact strength, +23°C 15 kJ/m² ISO 179/1eA
Flexural modulus, 23°C 2430 MPa ISO 178
Thermal propertiesValueUnitTest Standard
ISO Data
Temp. of deflection under load, 1.80 MPa 114 °C ISO 75-1/-2
Coeff. of linear therm. expansion, parallel 70 E-6/K ISO 11359-1/-2
Burning behav. at thickness h V-1 class IEC 60695-11-10
Thickness tested 0.7 mm -
ASTM Data
DTUL @ 264 psi 120 °C ASTM D 648
Electrical propertiesValueUnitTest Standard
ISO Data
Relative permittivity, 100Hz 2.9 - IEC 60250
Relative permittivity, 1MHz 2.9 - IEC 60250
Dissipation factor, 100Hz 30 E-4 IEC 60250
Dissipation factor, 1MHz 40 E-4 IEC 60250
Volume resistivity >1E13 Ohm*m IEC 60093
Surface resistivity >1E15 Ohm IEC 60093
Electric strength 29 kV/mm IEC 60243-1
Other propertiesValueUnitTest Standard
ISO Data
Density 1080 kg/m³ ISO 1183
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Special Characteristics
Flame retardant
Applications
Electrical and Electronical
Regional Availability
North America, Europe, Asia Pacific
Disclaimer
Copyright M-Base Engineering+Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from M-Base; this is especially valid for claims of compensation resulting from consequential damages. M-Base explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: 2017-11-23 Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.