Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of XANTAR™ MX 2034 - PC - Mitsubishi Engineering-Plastics Corporation

Material Data Center offers the following functions for XANTAR™ MX 2034:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, cooling time calculation, CAE Interfaces

Check here, which other Xantar datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Extremely Low Viscosity, Molding Release, UV Stabilized

ISO 1043 PC

XANTAR Polycarbonate & Blends, your global partner for innovative added value
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 35 cm³/10min ISO 1133
Temperature 300 °C -
Load 1.2 kg -
Molding shrinkage, parallel 0.6 % ISO 294-4, 2577
Density of melt 1010 kg/m³ -
Thermal conductivity of melt 0.24 W/(m K) -
Spec. heat capacity of melt 1710 J/(kg K) -
Eff. thermal diffusivity 1.4E-7 m²/s -
Ejection temperature 144 °C -
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 2300 MPa ISO 527
Yield stress 60 MPa ISO 527
Yield strain 6 % ISO 527
Nominal strain at break >50 % ISO 527
Thermal propertiesValueUnitTest Standard
ISO Data
Temp. of deflection under load, 1.80 MPa 130 °C ISO 75-1/-2
Vicat softening temperature, B 145 °C ISO 306
Coeff. of linear therm. expansion, parallel 65 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. V-2 class IEC 60695-11-10
Burning Behav. at thickness h V-2 class IEC 60695-11-10
Thickness tested 0.8 mm -
Electrical propertiesValueUnitTest Standard
ISO Data
Relative permittivity, 100Hz 3 - IEC 62631-2-1
Relative permittivity, 1MHz 2.9 - IEC 62631-2-1
Dissipation factor, 100Hz 6.6 E-4 IEC 62631-2-1
Dissipation factor, 1MHz 92 E-4 IEC 62631-2-1
Volume resistivity >1E13 Ohm*m IEC 62631-3-1
Surface resistivity >1E15 Ohm IEC 62631-3-2
Electric strength 29 kV/mm IEC 60243-1
Comparative tracking index 225 - IEC 60112
Other propertiesValueUnitTest Standard
Water absorption 0.35 % Sim. to ISO 62
Density 1200 kg/m³ ISO 1183
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 300 °C ISO 294
Injection Molding, mold temperature 90 °C ISO 294
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 110 °C -
Pre-drying - Time 4 h -
Processing humidity ≤0.03 % -
Melt temperature 270 - 290 °C -
Mold temperature 70 - 100 °C -
Zone 1 255 - 265 °C -
Zone 2 265 - 275 °C -
Zone 3 270 - 280 °C -
Nozzle temperature 260 - 270 °C -
Diagrams
Stress-strain , XANTAR™ MX 2034, PC, Mitsubishi EP
Secant modulus-strain , XANTAR™ MX 2034, PC, Mitsubishi EP
Specific volume-temperature (pvT) , XANTAR™ MX 2034, PC, Mitsubishi EP
Characteristics
Processing
Injection Molding
Delivery form
Pellets
Additives
Release agent
Special Characteristics
U.V. stabilized or stable to weather, Heat stabilized or stable to heat, Transparent
Regional Availability
Other text information
Injection molding
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.