Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of NORYL GTX™ Resin GTX830 - Asia - (PPE+PA*)-GF30 - Saudi Basic Industries Corporation (SABIC)

Material Data Center offers the following functions for NORYL GTX™ Resin GTX830 - Asia:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Noryl datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
NORYL GTX™ 830 resin is a 30% glass reinforced alloy of Polyphenylene Ether (PPE) + Polyamide (PA). This injection moldable grade has high stiffness (flexural modulus 8200 MPa), excellent chemical resistance, and high heat resistance. NORYL GTX GTX830 resin is an excellent candidate for a wide variety of applications including automotive under the bonnet applications and water meter housings.

UL Yellow Card Link E207780-104248654
Mechanical propertiesValueUnitTest Standard
ASTM Data
Tensile Strength at Yield 151 MPa ASTM D 638
Tensile Strength at Break 158 MPa ASTM D 638
Elongation at Break 7 % ASTM D 638
Rockwell Hardness R 120 - ASTM D 785
Izod Impact notched, 1/8 in 106 J/m ASTM D 256
Izod Impact notched, Low-Temperature 80 J/m ASTM D 256
Temperature -30 °C -
Thermal propertiesValueUnitTest Standard
ISO Data
Burning behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.5 mm -
ASTM Data
Vicat Temperature 248 °C ASTM D 1525
Other propertiesValueUnitTest Standard
Water Absorption, 24hr 0.5 % ASTM D 570
Density 1330 kg/m³ ASTM D 792
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 95 - 105 °C -
Pre-drying - Time 3 - 4 h -
Processing humidity ≤0.07 % -
Melt temperature 280 - 305 °C -
Mold temperature 75 - 120 °C -
Zone 1 265 - 305 °C -
Zone 2 270 - 305 °C -
Zone 3 275 - 305 °C -
Screw speed 20 - 100 rpm -
Back pressure 0.3 - 1.4 MPa -
Characteristics
Processing
Injection Molding
Applications
Automotive
Regional Availability
Asia Pacific
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.