Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VESTAMID® L-GB30 - PA12-GB30 - Evonik Operations GmbH

Material Data Center offers the following functions for VESTAMID® L-GB30:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Vestamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明

Microglass bead-filled (30%) PA12 resin for the injection moulding of rigid, low-warpage and dimensionally accurate mouldings

VESTAMID® L-GB30 NC is a glass bead –reinforced heat stabilized Polyamide 12 for injection molding. The material contains about 30% microglass beads, an ageing protective agent and a processing aid for a fast and even form filling. Due to the reinforcement moldings from this compound exhibit a higher strength, an isotropic shrinkage and good heat resistance, excellent for gear housings for mechanical counting mechanisms (e.g.speedometers or water gauges).

Further advantages of VESTAMID® L-GB30 NC are the characterizing properties of PA12, e.g., low water absorption, good dimensional stability and nearly constant mechanical properties at changing ambient humidity.
  
VESTAMID® L-GB30 NC is supplied as cylindrical granules, ready for processing, in moisture-proof bags.
 
Pigmentation may affect values.

Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.
 
The results shown have been generated from a low number of production lots. Therefore, they are preliminary and not yet the result of a statistical evaluation. Therefore they must not be used to establish specifications.

For information about processing of VESTAMID®, please follow the general commendations about “Processing of VESTAMID® compounds”. 

FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.VESTAMID.COM

加工/物理特性干 / 已调节单位Test Standard
ISO数据
熔体体积流动速度, MVR 100 / * cm³/10min ISO 1133
温度 275 / * °C -
载荷 5 / * kg -
模塑收缩率, 平行 0.6 / * % ISO 294-4, 2577
模塑收缩率, 垂直 0.7 / * % ISO 294-4, 2577
机械性能干 / 已调节单位Test Standard
ISO数据
拉伸模量 2100 / 1800 MPa ISO 527
屈服应力 47 / 37 MPa ISO 527
屈服伸长率 5 / 5 % ISO 527
名义断裂伸长率 20 / >50 % ISO 527
拉伸蠕变模量, 1h * / 1600 MPa ISO 899-1
拉伸蠕变模量, 1000h * / 1100 MPa ISO 899-1
无缺口简支梁冲击强度, +23°C 160 / N kJ/m² ISO 179/1eU
Type of failure C / - - -
简支梁冲击强度, -30°C 160 / N kJ/m² ISO 179/1eU
Type of failure C / - - -
简支梁缺口冲击强度, +23°C 4.4 / 6 kJ/m² ISO 179/1eA
Type of failure C / C - -
简支梁缺口冲击强度, -30°C 6 / 6 kJ/m² ISO 179/1eA
Type of failure C / C - -
热性能干 / 已调节单位Test Standard
ISO数据
熔融温度, 10°C/min 178 / * °C ISO 11357-1/-3
热变形温度, 1.80 MPa 55 / * °C ISO 75-1/-2
热变形温度, 0.45 MPa 150 / * °C ISO 75-1/-2
维卡软化温度, B 155 / * °C ISO 306
线性热膨胀系数, 平行 130 / * E-6/K ISO 11359-1/-2
线性热膨胀系数, 垂直 130 / * E-6/K ISO 11359-1/-2
1.5mm名义厚度时的燃烧性 HB / * class IEC 60695-11-10
测试用试样的厚度 1.5 / * mm -
Yellow Card 现存 是的 / * - -
厚度为h时的燃烧性 HB / * class IEC 60695-11-10
测试用试样的厚度 0.8 / * mm -
Yellow Card 现存 是的 / * - -
电性能干 / 已调节单位Test Standard
ISO数据
相对介电常数., 100Hz 4.1 / 5 - IEC 62631-2-1
相对介电常数., 1MHz 3.5 / 4 - IEC 62631-2-1
介质损耗因子, 100Hz 310 / 600 E-4 IEC 62631-2-1
介质损耗因子, 1MHz 230 / 370 E-4 IEC 62631-2-1
体积电阻率 >1E13 / 2E12 Ohm*m IEC 62631-3-1
表面电阻率 * / 1E15 Ohm IEC 62631-3-2
介电强度 - / 36 kV/mm IEC 60243-1
相对漏电起痕指数 600 / 600 - IEC 60112
其它性能干 / 已调节单位Test Standard
吸水性 1.1 / * % 类似ISO 62
吸湿性 0.5 / * % 类似ISO 62
密度 1250 / 1260 kg/m³ ISO 1183
函数
粘度-剪切速度 , VESTAMID® L-GB30, PA12-GB30, Evonik
剪切应力-剪切速度 , VESTAMID® L-GB30, PA12-GB30, Evonik
动态剪切模量-温度 , VESTAMID® L-GB30 (烘干), PA12-GB30, Evonik
应力-应变.  , VESTAMID® L-GB30 (烘干), PA12-GB30, Evonik
正割模量-应变.  , VESTAMID® L-GB30 (烘干), PA12-GB30, Evonik
应力-应变(等时的) 23°C, VESTAMID® L-GB30 (状况), PA12-GB30, Evonik
蠕变模量-时间. 23°C, VESTAMID® L-GB30 (状况), PA12-GB30, Evonik
蠕变曲线 23°C, VESTAMID® L-GB30 (状况), PA12-GB30, Evonik
典型数据
加工方法
注塑
供货形式
粒料, 自然色
添加剂
润滑剂
特殊性能
经热稳处理的/耐热的
特征
低翘曲
地区供应
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.