Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of PLEXIGLAS® 7M - PMMA - Röhm GmbH

Material Data Center offers the following functions for PLEXIGLAS® 7M:
unit conversion, PDF datasheet print, comparison with other plastics, flow length calculation, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Plexiglas datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts

Productprofil:

PLEXIGLAS® 7M molding compound is based on polymethyl methacrylate (PMMA).

 

Besides showing the familiar properties of PLEXIGLAS® 7H molding compounds, such as

 

  • excellent light transmission and brilliance
  • excellent weatherability
  • high mechanical strength, surface hardness and abrasion resistance.

 

PLEXIGLAS® 7M is special in that it

 

  • better flowing behavior,
  • AMECA listing.

Application:

PLEXIGLAS® 7M is particularly suitable for extruding profiles and panels for use in lighting engineering.

Example:

lighting fixtures, displays and similar extruded items for technical purposes.

Processing:

PLEXIGLAS® 7M can be processed on extruders with 3-zone general purpose screws for thermoplastics.

Physical Form / Packaging:

PLEXIGLAS® molding compound is supplied as pellets of uniform size in two-ply, 25kg polyethylene bags; other packaging on request.

Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 2.9 cm³/10min ISO 1133
Temperature 230 °C -
Load 3.8 kg -
Density of melt 1060 kg/m³ -
Thermal conductivity of melt 0.181 W/(m K) -
Spec. heat capacity of melt 2440 J/(kg K) -
Eff. thermal diffusivity 6.99E-8 m²/s -
Ejection temperature 85 °C -
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 3200 MPa ISO 527
Stress at break 69 MPa ISO 527
Strain at break 4 % ISO 527
Charpy impact strength, +23°C 20 kJ/m² ISO 179/1eU
Thermal propertiesValueUnitTest Standard
ISO Data
Glass transition temperature, 10°C/min 108 °C ISO 11357-1/-2
Vicat softening temperature, B 104 °C ISO 306
Coeff. of linear therm. expansion, parallel 80 E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB class IEC 60695-11-10
Thickness tested 1.6 mm -
Yellow Card available yes - -
Oxygen index 17.2 % ISO 4589-1/-2
Electrical propertiesValueUnitTest Standard
ISO Data
Relative permittivity, 100Hz 3.7 - IEC 62631-2-1
Relative permittivity, 1MHz 2.8 - IEC 62631-2-1
Dissipation factor, 100Hz 500 E-4 IEC 62631-2-1
Dissipation factor, 1MHz 200 E-4 IEC 62631-2-1
Volume resistivity >1E13 Ohm*m IEC 62631-3-1
Surface resistivity 1E13 Ohm IEC 62631-3-2
Optical propertiesValueUnitTest Standard
ISO Data
Luminous transmittance 92 % ISO 13468-1, -2
Other propertiesValueUnitTest Standard
Water absorption 2 % Sim. to ISO 62
Humidity absorption 0.6 % Sim. to ISO 62
Density 1190 kg/m³ ISO 1183
Material specific propertiesValueUnitTest Standard
ISO Data
Viscosity number 62 cm³/g ISO 307, 1157, 1628
Test specimen productionValueUnitTest Standard
ISO Data
Processing conditions acc. ISO 8257 - ISO ....-2
Injection Molding, melt temperature 254 °C ISO 294
Injection Molding, mold temperature 64 °C ISO 294
Injection Molding, injection velocity 195 mm/s ISO 294
Diagrams
Viscosity-shear rate , PLEXIGLAS® 7M, PMMA, Röhm
Shearstress-shear rate , PLEXIGLAS® 7M, PMMA, Röhm
Dynamic Shear modulus-temperature , PLEXIGLAS® 7M, PMMA, Röhm
Stress-strain , PLEXIGLAS® 7M, PMMA, Röhm
Secant modulus-strain , PLEXIGLAS® 7M, PMMA, Röhm
Tensile modulus-temperature , PLEXIGLAS® 7M, PMMA, Röhm
Characteristics
Processing
Injection Molding, Profile Extrusion, Sheet Extrusion, Other Extrusion
Delivery form
Pellets
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather, Transparent
Regional Availability
North America, Europe, Asia Pacific, South and Central America, Near East/Africa
Other text information
Profile extrusion
PREPROCESSING
Predrying temperature: max. 94 °C
Predrying time in a desiccant-type drier: 2 - 3 h
PROCESSING
Melt temperature: 220 - 260 °C
Die temperature: 220 - 260 °C
Sheet extrusion
PREPROCESSING
Predrying temperature: max. 94 °C
Predrying time in a desiccant-type drier: 2 - 3 h
PROCESSING
Melt temperature: 220 - 260 °C
Die temperature: 220 - 260 °C
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com