Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of SILTEM™ Resin STM1500 - Americas - PEI - Saudi Basic Industries Corporation (SABIC)

Material Data Center offers the following functions for SILTEM™ Resin STM1500 - Americas:
unit conversion, PDF datasheet print, comparison with other plastics

Check here, which other Siltem datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
材料文字说明
SILTEM™ STM1500 resin is a flexible polyetherimide(PEI)-siloxane copolymer for cable and wire coatings. RoHS compliant.
加工/物理特性价值单位Test Standard
ASTM数据
熔融指数, MFI 12 g/10min ASTM D 1238
温度 295 °C -
负载 6.6 kg -
机械性能价值单位Test Standard
ASTM数据
屈服应力 28 MPa ASTM D 638
断裂伸长率 100 % ASTM D 638
Taber耐磨损性 26 mg/1000 cycles ASTM D 1044
电性能价值单位Test Standard
ASTM数据
电介质强度, 短时 16.3 kV/mm ASTM D 149
耗散因素, 60 Hz 0.01 - ASTM D 150
电介质常数, 60 Hz 3.01 - ASTM D 150
表面电阻率 1E15 Ohm ASTM D 257
体积电阻率 >1E15 Ohm*cm ASTM D 257
其它性能价值单位Test Standard
密度 1180 kg/m³ ASTM D 792
加工推荐(注塑)价值单位Test Standard
预干燥-温度 105 °C -
预干燥-时间 4 - 6 h -
加工湿度 ≤0.02 % -
注塑熔体温度 300 - 320 °C -
模具温度 65 - 95 °C -
1区 295 - 315 °C -
2区 295 - 315 °C -
3区 295 - 315 °C -
螺杆转速 50 - 100 rpm -
背压 0.3 - 0.7 MPa -
典型数据
加工方法
注塑
Certifications
RoHS
地区供应
北美
权利义务的法律声明
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com