Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of VALOX™ FR Resin ENH4550 - Asia - PBT-GF25 - Saudi Basic Industries Corporation (SABIC)

Material Data Center offers the following functions for VALOX™ FR Resin ENH4550 - Asia:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, cooling time calculation, parameters for material models, CAE Interfaces

Check here, which other Valox datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Informação do produto
VALOX ENH4550 is a 25% glass reinforced, non-chlorinated/brominated flame retardant Polybutylene Terephthalate (PBT) injection moldable grade with excellent chemical resistance. It has a UL94V0@0.30mm and 5VA@2.0mm flame rating. This is a good candidate for a variety of applications needing a sustainable FR PBT solution.

UL Yellow Card Link E207780-101458997
Características de processamento/físicasValorUnidadeMétodo de ensaio
ISO Dados
Índice de fluidez volumétrico, MVR 18 cm³/10min ISO 1133
Temperatura 265 °C -
Carga 5 kg -
Densidade do fundido 1330 kg/m³ -
Condutividade térmica do fundido 0.26 W/(m K) -
Capacidade térmica específica do fundido 1700 J/(kg K) -
Temperatura de ejeção 170 °C -
ASTM Dados
Índice de fluidez, MFI 27 g/10min ASTM D 1238
Temperatura 265 °C -
Carga 5 kg -
Propriedades mecânicasValorUnidadeMétodo de ensaio
ISO Dados
Módulo de tração 10400 MPa ISO 527
Tensão no escoamento 112 MPa ISO 527
Deformação no escoamento 2 % ISO 527
Tensão na ruptura 112 MPa ISO 527
Deformação na ruptura 2 % ISO 527
Módulo de flexão 9200 MPa ISO 178
Res. impacto Charpy c/entalhe, +23°C 5 kJ/m² ISO 179/1eA
Izod impact strength, +23°C, 4mm 40 kJ/m² ISO 180/1U
Izod impact strength, -30°C, 4mm 35 kJ/m² ISO 180/1U
Res. impacto Izod c/entalhe, +23°C, 4mm 8 kJ/m² ISO 180/1A
Res. impacto Izod c/entalhe, -30°C, 4mm 8 kJ/m² ISO 180/1A
Dureza Rockwell R 124 - ISO 2039-2
Ball indentation hardness 174 MPa ISO 2039-1
ASTM Dados
Módulo de tração 10300 MPa ASTM D 638
Resistência à tração no escoamento 115 MPa ASTM D 638
Resistência à tração na ruptura 115 MPa ASTM D 638
Alongamento no escoamento 2 % ASTM D 638
Deformação na ruptura 2 % ASTM D 638
Módulo de flexão 8800 MPa ASTM D 790
Impacto Izod com entalhe, 1/8 in 70 J/m ASTM D 256
Impacto Izod com entalhe, baixa temperatura 65 J/m ASTM D 256
Temperatura -30 °C -
Resistência ao Impacto Izod, 1/8 in 550 J/m ASTM D 256
Propriedades térmicasValorUnidadeMétodo de ensaio
ISO Dados
Temperatura de deflexão térmica, 1.80 MPa 207 °C ISO 75-1/-2
Temperatura de deflexão térmica , 0.45 MPa 220 °C ISO 75-1/-2
Temperatura de amolecimento Vicat , A 220 °C ISO 306
Temperatura de amolecimento Vicat, B 207 °C ISO 306
Temperatura de amolecimento Vicat, 120°C/h 50N 208 °C ISO 306
Coef. de expansão térmica linear, paralelo 27.5 E-6/K ISO 11359-1/-2
Coef. de expansão térmica linear, perpend. 154 E-6/K ISO 11359-1/-2
Flamabilidade a espessura h V-0 class IEC 60695-11-10
Espessuras do tubo de teste 0.3 mm -
Flamabilidade 5V a espessura h 5VA class IEC 60695-11-20
Espessuras do tubo de teste 2.0 mm -
Glow Wire Flammability Index (GWFI) 960 °C IEC 60695-2-12
Glow Wire Flammability Index (GWFI) 960 °C IEC 60695-2-12
Glow Wire Ignition Temperature (GWIT) 775 °C IEC 60695-2-13
GWIT - thickness tested (1) 1 mm -
Glow Wire Ignition Temperature (GWIT) 775 °C IEC 60695-2-13
GWIT - thickness tested (3) 3 mm -
ASTM Dados
DTUL @ 66 psi 220 °C ASTM D 648
DTUL @ 264 psi 205 °C ASTM D 648
Temperatura de amolecimento Vicat 205 °C ASTM D 1525
Propriedades elétricasValorUnidadeMétodo de ensaio
ISO Dados
Constante dielétrica, 1MHz 3.4 - IEC 62631-2-1
Fator de dissipação dielétrica, 1MHz 1200 E-4 IEC 62631-2-1
Resistividade volumétrica específica 1E13 Ohm*m IEC 62631-3-1
Resistividade superficial específica >1E15 Ohm IEC 62631-3-2
Resistência elétrica 30 kV/mm IEC 60243-1
Índice comparativo de linha de fuga 300 - IEC 60112
ASTM Dados
Resistência elétrica, tempo curto 20 kV/mm ASTM D 149
Fator de dissipação dielétrica, 1 MHz 0.12 - ASTM D 150
Constante dielétrica, 1 MHz 3.4 - ASTM D 150
Resistividade volumétrica específica 1E15 Ohm*cm ASTM D 257
Outras propriedadesValorUnidadeMétodo de ensaio
Absorção de água 0.23 % Sim. to ISO 62
Absorção de umidade 0.06 % Sim. to ISO 62
Densidade 1520 kg/m³ ISO 1183
Densidade 1520 kg/m³ ASTM D 792
Recomendação de processamento Moldagem por injeçãoValorUnidadeMétodo de ensaio
Pré-secagem - temperatura 110 - 120 °C -
Pré-secagem - tempo 2 - 4 h -
Umidade do processamento ≤0.02 % -
Temperatura da massa 245 - 260 °C -
Temperatura do molde 40 - 100 °C -
Temperatura - zona de alimentação 40 - 60 °C -
Zona 1 230 - 240 °C -
Zona 2 235 - 250 °C -
Zona 3 240 - 260 °C -
Diagrama
Viscosidade - taxa de cisalhamento , VALOX™ FR Resin ENH4550 - Asia, PBT-GF25, SABIC
Tensão de cisalhamento - taxa de cisalhamento , VALOX™ FR Resin ENH4550 - Asia, PBT-GF25, SABIC
Volume específico - temperatura (pvT) , VALOX™ FR Resin ENH4550 - Asia, PBT-GF25, SABIC
Características
Processamento
Moldagem por injeção
Aditivos
Anti-chama
Características especiais
Retardante de chama
Resistência Química
Resistência química geral
Disponibilidade regional
Ásia Pacífico
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.