Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of NORYL™ Resin FE1630PW - Asia - (PPE+PS)-GF30 - Saudi Basic Industries Corporation (SABIC)

Material Data Center offers the following functions for NORYL™ Resin FE1630PW - Asia:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Noryl datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
商品の説明文
NORYL™ FE1630PW resin is a 30% glass reinforced blend of polyphenylene ether (PPE) + crystal clear polystyrene (ccPS). This injection moldable material is FC EU, FDA food contact compliant, NSF/ANSI 61*ACS, WRAS, KTW, and W270 listed for global potable water use. NORYL FE1630PW resin exhibits excellent long-term hydrolytic stability, very low moisture absorption, heat / hot water resistance and is an excellent candidate for a variety of water management applications such as pump housings, impellers, shower/faucet, membrane housings and valves. *NSF certification is color dependent.
Processing/Physical Characteristics単位テスト基準
ISO データ
メルトボリュームレイト, MVR 30 cm³/10min ISO 1133
温度 300 °C -
荷重 10 kg -
ASTM数据
メルトフローレイト, MFI 9 g/10min ASTM D 1238
温度 300 °C -
荷重 5 kg -
機械的特性単位テスト基準
ISO データ
引張弾性率 9600 MPa ISO 527
破壊応力 133 MPa ISO 527
破壊ひずみ 2.5 % ISO 527
曲げ弾性率 8120 MPa ISO 178
シャルピー衝撃強さ, +23°C 30 kJ/m² ISO 179/1eU
シャルピー衝撃強さ, -30゚C 30 kJ/m² ISO 179/1eU
ノッチ付きシャルピー衝撃強さ, +23°C 10 kJ/m² ISO 179/1eA
ノッチ付きシャルピー衝撃強さ, -30゚C 9 kJ/m² ISO 179/1eA
Izod impact strength, +23°C, 4mm 30 kJ/m² ISO 180/1U
Izod impact strength, -30°C, 4mm 30 kJ/m² ISO 180/1U
ノッチ付きアイゾット衝撃強さ, +23°C, 4mm 8 kJ/m² ISO 180/1A
ノッチ付きアイゾット衝撃強さ, -30°C, 4mm 7 kJ/m² ISO 180/1A
Ball indentation hardness 240 MPa ISO 2039-1
ASTM数据
引張弾性率 9570 MPa ASTM D 638
破壊応力 134 MPa ASTM D 638
破断伸び 2.4 % ASTM D 638
曲げ弾性率 7760 MPa ASTM D 790
ノッチ付きIzod衝撃強さ, 1/8 in 85 J/m ASTM D 256
ノッチ付きIzod衝撃強さ, Low-Temperature 75 J/m ASTM D 256
温度 -30 °C -
アイゾット衝撃試験, 1/8 in 505 J/m ASTM D 256
熱的特性単位テスト基準
ISO データ
ビカット軟化温度, A 165 °C ISO 306
ビカット軟化温度, B 154 °C ISO 306
ビカット軟化温度, 120°C/h 50N 158 °C ISO 306
ASTM数据
DTUL @ 264 psi 145 °C ASTM D 648
その他の特性.単位テスト基準
吸水率. 0.2 % Sim. to ISO 62
吸湿率 0.06 % Sim. to ISO 62
密度. 1300 kg/m³ ISO 1183
Processing Recommendation Injection Molding単位テスト基準
Pre-drying - Temperature 100 - 120 °C -
Pre-drying - Time 2 - 4 h -
Processing humidity ≤0.02 % -
樹脂温度 290 - 320 °C -
金型温度 80 - 120 °C -
Feed temperature 60 - 80 °C -
Zone 1 270 - 280 °C -
Zone 2 280 - 300 °C -
Zone 3 300 - 310 °C -
特殊な特性
成形加工法.
射出成形.
耐薬品性
Hydrolytically Stable
Certifications
Food contact, Food approval FDA 21 CFR
領域別の利用可能性
アジア/太平洋地域.
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.