Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of TROGAMID® CX7323 NC - PAPACM12 - Evonik Operations GmbH

Material Data Center offers the following functions for TROGAMID® CX7323 NC:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, parameters for material models, CAE Interfaces

Check here, which other Trogamid datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Microcrystalline, permanently transparent polyamide

TROGAMID® CX7323 is a microcrystalline transparent polyamide for the manufacture of parts according the injection molding procedure.

The crystallites are so small, that they do not scatter visible light, and the material appears transparent to the human eye. The crystalline structure causes the excellent crack resistance for this polymer.

TROGAMID® CX7323 is supplied as spherical pellets in polyethylene packaging.

Deviations of molds or in processing are possible to a certain extent, if they are required by the cavity or the process itself.


Pigmentation may affect values.

For information about processing of TROGAMID®, please follow the general commendations about “Processing of TROGAMID® compounds”. 
 
FOR FURTHER INFORMATION PLEASE CONTACT US AT EVONIK-HP@EVONIK.COM
OR VISIT OUR PRODUCT AT  WWW.TROGAMID.COM

Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 8.2 / * cm³/10min ISO 1133
Temperature 280 / * °C -
Load 2.16 / * kg -
Molding shrinkage, parallel 0.7 / * % ISO 294-4, 2577
Molding shrinkage, normal 0.8 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 1400 / - MPa ISO 527
Yield stress 60 / - MPa ISO 527
Yield strain 8 / - % ISO 527
Nominal strain at break >50 / - % ISO 527
Tensile creep modulus, 1h * / 1300 MPa ISO 899-1
Tensile creep modulus, 1000h * / 700 MPa ISO 899-1
Charpy impact strength, +23°C N / - kJ/m² ISO 179/1eU
Charpy impact strength, -30°C N / - kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 11 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Charpy notched impact strength, -30°C 11 / - kJ/m² ISO 179/1eA
Type of failure C / - - -
Shore D hardness 81 / * - ISO 7619-1
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 250 / * °C ISO 11357-1/-3
Glass transition temperature, 10°C/min 140 / * °C ISO 11357-1/-2
Temp. of deflection under load, 1.80 MPa 108 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 122 / * °C ISO 75-1/-2
Vicat softening temperature, B 130 / * °C ISO 306
Coeff. of linear therm. expansion, parallel 90 / * E-6/K ISO 11359-1/-2
Coeff. of linear therm. expansion, normal 90 / * E-6/K ISO 11359-1/-2
Burning Behav. at 1.5 mm nom. thickn. HB / * class IEC 60695-11-10
Thickness tested 1.5 / * mm -
Yellow Card available yes / * - -
Burning Behav. at thickness h HB / * class IEC 60695-11-10
Thickness tested 0.8 / * mm -
Yellow Card available yes / * - -
Electrical propertiesdry / condUnitTest Standard
ISO Data
Relative permittivity, 100Hz 3.6 / - - IEC 62631-2-1
Relative permittivity, 1MHz 3.2 / - - IEC 62631-2-1
Dissipation factor, 100Hz 115 / - E-4 IEC 62631-2-1
Dissipation factor, 1MHz 325 / - E-4 IEC 62631-2-1
Volume resistivity >1E13 / - Ohm*m IEC 62631-3-1
Surface resistivity * / 1E13 Ohm IEC 62631-3-2
Electric strength 27 / - kV/mm IEC 60243-1
Comparative tracking index 600 / - - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 3.5 / * % Sim. to ISO 62
Humidity absorption 1.5 / * % Sim. to ISO 62
Density 1020 / - kg/m³ ISO 1183
Diagrams
Dynamic Shear modulus-temperature , TROGAMID® CX7323 NC (dry), PAPACM12, Evonik
Stress-strain (isochronous) 23°C, TROGAMID® CX7323 NC (dry), PAPACM12, Evonik
Creep modulus-time 23°C, TROGAMID® CX7323 NC (dry), PAPACM12, Evonik
Creep curve 23°C, TROGAMID® CX7323 NC (dry), PAPACM12, Evonik
Stress-strain (isochronous) 40°C, TROGAMID® CX7323 NC (dry), PAPACM12, Evonik
Creep modulus-time 40°C, TROGAMID® CX7323 NC (dry), PAPACM12, Evonik
Creep curve 40°C, TROGAMID® CX7323 NC (dry), PAPACM12, Evonik
Specific volume-temperature (pvT) , TROGAMID® CX7323 NC, PAPACM12, Evonik
Spec. enthalpy/mass-temp. (DSC) , TROGAMID® CX7323 NC, PAPACM12, Evonik
Characteristics
Processing
Injection Molding, Film Extrusion, Profile Extrusion, Sheet Extrusion, Other Extrusion
Delivery form
Pellets, Natural Color
Special Characteristics
Light stabilized or stable to light, U.V. stabilized or stable to weather, Transparent
Chemical Resistance
Environmental Stress Crack Resistance
Regional Availability
North America, Europe, Asia Pacific, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.