Any use of this information falls under the rules of our
disclaimer.
Processing/Physical Characteristics | Value | Unit | Test Standard |
ISO Data |
Melt volume-flow rate, MVR |
6 |
cm³/10min |
ISO 1133 |
Temperature |
300 |
°C |
- |
Load |
1.2 |
kg |
- |
Molding shrinkage, parallel |
0.7 |
% |
ISO 294-4, 2577 |
Molding shrinkage, normal |
0.7 |
% |
ISO 294-4, 2577 |
Mechanical properties | Value | Unit | Test Standard |
ISO Data |
Tensile Modulus |
2300 |
MPa |
ISO 527 |
Yield stress |
66 |
MPa |
ISO 527 |
Yield strain |
6.2 |
% |
ISO 527 |
Nominal strain at break |
>50 |
% |
ISO 527 |
Stress at break |
60 |
MPa |
ISO 527 |
Strain at break |
60 |
% |
ISO 527 |
Flexural modulus, 23°C |
2400 |
MPa |
ISO 178 |
Flexural strength |
99 |
MPa |
ISO 178 |
Charpy impact strength, +23°C |
N |
kJ/m² |
ISO 179/1eU |
Charpy notched impact strength, +23°C, 3mm |
32 |
kJ/m² |
ISO 179/1eA |
Izod notched impact strength, +23°C |
50[1] |
kJ/m² |
ISO 180/1A |
Puncture - maximum force, +23°C |
5100 |
N |
ISO 6603-2 |
Puncture - maximum force, -30°C |
6100 |
N |
ISO 6603-2 |
Puncture energy, +23°C |
50 |
J |
ISO 6603-2 |
Puncture energy, -30°C |
55 |
J |
ISO 6603-2 |
Ball indentation hardness |
120 |
MPa |
ISO 2039-1 |
Thermal properties | Value | Unit | Test Standard |
ISO Data |
Temp. of deflection under load, 1.80 MPa |
121 |
°C |
ISO 75-1/-2 |
Temp. of deflection under load, 0.45 MPa |
136 |
°C |
ISO 75-1/-2 |
Vicat softening temperature, B |
142 |
°C |
ISO 306 |
Burning behav. at thickness h |
V-0 |
class |
IEC 60695-11-10 |
Thickness tested |
1.0 |
mm |
- |
Burning behav. 5V at thickness h |
5VA |
class |
IEC 60695-11-20 |
Thickness tested |
3.0 |
mm |
- |
Oxygen index |
39 |
% |
ISO 4589-1/-2 |
Glow Wire Flammability Index (GWFI) |
960 |
°C |
IEC 60695-2-12 |
GWFI - thickness tested (1) |
0.75 |
mm |
- |
Glow Wire Flammability Index (GWFI) |
960 |
°C |
IEC 60695-2-12 |
GWFI - thickness tested (2) |
1.5 |
mm |
- |
Glow Wire Flammability Index (GWFI) |
960 |
°C |
IEC 60695-2-12 |
GWFI - thickness tested (3) |
3 |
mm |
- |
Glow Wire Ignition Temperature (GWIT) |
850 |
°C |
IEC 60695-2-13 |
GWIT - thickness tested (1) |
0.75 |
mm |
- |
Glow Wire Ignition Temperature (GWIT) |
850 |
°C |
IEC 60695-2-13 |
GWIT - thickness tested (2) |
1.5 |
mm |
- |
Glow Wire Ignition Temperature (GWIT) |
850 |
°C |
IEC 60695-2-13 |
GWIT - thickness tested (3) |
3 |
mm |
- |
Optical properties | Value | Unit | Test Standard |
ISO Data |
Haze |
1 |
- |
ISO 14782 |
Luminous transmittance |
89 |
% |
ISO 13468-1, -2 |
Other Standards[S] |
Index of Refraction |
1.58 |
- |
ISO 489 |
S: | These properties are reported by the producer according standards that are different to our defaults. |
Other properties | Value | Unit | Test Standard |
Density |
1200 |
kg/m³ |
ISO 1183 |
Processing Recommendation Injection Molding | Value | Unit | Test Standard |
Pre-drying - Temperature |
120 |
°C |
- |
Pre-drying - Time |
4 |
h |
- |
Melt temperature |
280 - 320 |
°C |
- |
Mold temperature |
80 |
°C |
- |
Characteristics
Processing
Injection Molding
Additives
Release agent
Special Characteristics
Flame retardant, U.V. stabilized or stable to weather, Transparent
Certifications
Contains renewable resources
Regional Availability
North America, Europe, Asia Pacific, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com