Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Makrolon® 3207 - PC - Covestro Deutschland AG

Material Data Center offers the following functions for Makrolon® 3207:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Makrolon datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
  • MVR (300 °C/1.2 kg) 4.0 cm³/10 min
  • general purpose
  • high viscosity
  • UV stabilized
  • easy release
  • developed for safety goggles
Processing/Physical CharacteristicsValueUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 4 cm³/10min ISO 1133
Temperature 300 °C -
Load 1.2 kg -
Molding shrinkage, parallel 0.7 % ISO 294-4, 2577
Molding shrinkage, normal 0.7 % ISO 294-4, 2577
Mechanical propertiesValueUnitTest Standard
ISO Data
Tensile Modulus 2270 MPa ISO 527
Yield stress 62 MPa ISO 527
Yield strain 6.5 % ISO 527
Nominal strain at break >50 % ISO 527
Flexural modulus, 23°C 2400 MPa ISO 178
Flexural strength 97 MPa ISO 178
Charpy impact strength, +23°C N kJ/m² ISO 179/1eU
Charpy impact strength, -30°C N kJ/m² ISO 179/1eU
Izod notched impact strength, +23°C 75 kJ/m² ISO 180/1A
Izod notched impact strength 20 kJ/m² ISO 180/1A
Temperature -30 °C -
Puncture - maximum force, +23°C 5720 N ISO 6603-2
Puncture energy, +23°C 60 J ISO 6603-2
Thermal propertiesValueUnitTest Standard
ISO Data
Glass transition temperature, 10°C/min 151 °C ISO 11357-1/-2
Temp. of deflection under load, 1.80 MPa 130 °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 141 °C ISO 75-1/-2
Vicat softening temperature, B 149 °C ISO 306
Optical propertiesValueUnitTest Standard
ISO Data
Haze 0.2 - ISO 14782
Luminous transmittance 89 % ISO 13468-1, -2
Other propertiesValueUnitTest Standard
Density 1190 kg/m³ ISO 1183
Film PropertiesValueUnitTest Standard
ISO Data
Thickness of specimen 3 mm -
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 120 °C -
Pre-drying - Time 2 - 3 h -
Processing humidity ≤0.02 % -
Melt temperature 290 - 330 °C -
Mold temperature 80 - 120 °C -
Zone 1 260 - 270 °C -
Zone 2 280 - 290 °C -
Zone 3 290 - 300 °C -
Nozzle temperature 300 - 310 °C -
Back pressure 5 - 15 MPa -
Characteristics
Processing
Injection Molding
Additives
Release agent
Special Characteristics
U.V. stabilized or stable to weather, Transparent
Applications
General Purpose
Regional Availability
North America, Europe, Asia Pacific, South and Central America, Near East/Africa
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com