Any use of this information falls under the rules of our
disclaimer.
Processing/Physical Characteristics | Value | Unit | Test Standard |
ISO Data |
Melt flow index, MFI |
10 |
g/10min |
ISO 1133 |
Temperature |
260 |
°C |
- |
Load |
5 |
kg |
- |
Molding shrinkage, parallel |
0.6 |
% |
ISO 294-4, 2577 |
Molding shrinkage, normal |
0.6 |
% |
ISO 294-4, 2577 |
ASTM Data |
Melt Flow Index, MFI |
2.8 |
g/10min |
ASTM D 1238 |
Temperature |
250 |
°C |
- |
Load |
2.16 |
kg |
- |
Mold Shrinkage, MD |
0.006 |
mm/mm |
ASTM D 955 |
Mold Shrinkage, TD |
0.006 |
mm/mm |
ASTM D 955 |
Mechanical properties | Value | Unit | Test Standard |
ISO Data |
Tensile Modulus |
2000 |
MPa |
ISO 527 |
Yield stress |
45 |
MPa |
ISO 527 |
Yield strain |
4.2 |
% |
ISO 527 |
Stress at break |
48 |
MPa |
ISO 527 |
Strain at break |
100 |
% |
ISO 527 |
Flexural modulus, 23°C |
2230 |
MPa |
ISO 178 |
Flexural strength |
75 |
MPa |
ISO 178 |
Charpy notched impact strength, +23°C |
60[1] |
kJ/m² |
ISO 179/1eA |
Charpy notched impact strength, -30°C |
53[1] |
kJ/m² |
ISO 179/1eA |
Izod notched impact strength, +23°C |
57[1] |
kJ/m² |
ISO 180/1A |
Izod notched impact strength |
38[1] |
kJ/m² |
ISO 180/1A |
Temperature |
-40 |
°C |
- |
Rockwell hardness |
R 117 |
- |
ISO 2039-2 |
ASTM Data |
Tensile Modulus |
2228 |
MPa |
ASTM D 638 |
Tensile Strength at Yield |
51 |
MPa |
ASTM D 638 |
Tensile Strength at Break |
52 |
MPa |
ASTM D 638 |
Elongation at Yield |
4.2 |
% |
ASTM D 638 |
Elongation at Break |
128 |
% |
ASTM D 638 |
Flexural Modulus |
2263 |
MPa |
ASTM D 790 |
Flexural Strength |
85.3 |
MPa |
ASTM D 790 |
Rockwell Hardness |
R 117 |
- |
ASTM D 785 |
Izod Impact notched, 1/8 in |
736 |
J/m |
ASTM D 256 |
Izod Impact notched, 1/4 in |
520 |
J/m |
ASTM D 256 |
Izod Impact notched, Low-Temperature |
500 |
J/m |
ASTM D 256 |
Temperature |
-30 |
°C |
- |
Thermal properties | Value | Unit | Test Standard |
ISO Data |
Temp. of deflection under load, 1.80 MPa |
94[2] |
°C |
ISO 75-1/-2 |
Temp. of deflection under load, 0.45 MPa |
113[2] |
°C |
ISO 75-1/-2 |
Vicat softening temperature, B |
113 |
°C |
ISO 306 |
Coeff. of linear therm. expansion, parallel |
78 |
E-6/K |
ISO 11359-1/-2 |
Coeff. of linear therm. expansion, normal |
84 |
E-6/K |
ISO 11359-1/-2 |
ASTM Data |
Coefficient of Thermal Expansion, MD |
78 |
E-6/K |
ASTM D 696 |
Coefficient of Thermal Expansion, TD |
84 |
E-6/K |
ASTM D 696 |
DTUL @ 66 psi |
120[3] |
°C |
ASTM D 648 |
DTUL @ 264 psi |
104[3] |
°C |
ASTM D 648 |
Vicat Temperature |
113 |
°C |
ASTM D 1525 |
Electrical properties | Value | Unit | Test Standard |
ISO Data |
Volume resistivity |
1E15 |
Ohm*m |
IEC 62631-3-1 |
Surface resistivity |
1E15 |
Ohm |
IEC 62631-3-2 |
ASTM Data |
Dielectric Strength, Short Time |
25 |
kV/mm |
ASTM D 149 |
Surface Resistivity |
1E15 |
Ohm |
ASTM D 257 |
Volume Resistivity |
1E17 |
Ohm*cm |
ASTM D 257 |
Other properties | Value | Unit | Test Standard |
Humidity absorption |
0.2 |
% |
Sim. to ISO 62 |
Density |
1110 |
kg/m³ |
ISO 1183 |
Density |
1110 |
kg/m³ |
ASTM D 792 |
Processing Recommendation Injection Molding | Value | Unit | Test Standard |
Pre-drying - Temperature |
80 - 100 |
°C |
- |
Pre-drying - Time |
4 - 6 |
h |
- |
Processing humidity |
≤0.02 |
% |
- |
Melt temperature |
240 - 260 |
°C |
- |
Mold temperature |
60 - 80 |
°C |
- |
Zone 1 |
240 - 260 |
°C |
- |
Zone 2 |
250 - 270 |
°C |
- |
Zone 3 |
250 - 270 |
°C |
- |
Nozzle temperature |
250 - 280 |
°C |
- |
Characteristics
Processing
Injection Molding
Applications
Automotive, General Purpose
Regional Availability
North America, Europe, Asia Pacific, South and Central America
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com